Copper Alloy No. C95600Aluminum Bronze CDA 956Chemical Composition % by weight
Element Nominal Minimum Maximum Copper 90.3 88 Rem. Lead - - - Iron - - - Nickel (incl Co) - - .25 Aluminum 7 6 8 Manganese - - - Magnesium - - - Silicon 2.5 1.8 3.2 Zinc - - - Tin - - -
Cable connectors, pole line hardware, terminals, gears, worm gears, marine hardware, valve stems. Applications
M07 - As Continuous Cast
Hardness* Brinell Hardness (3000 kg load) 140 Tensile Strength** KSI 75 Yield Strength ** KSI (0.5% Ext. under load) 34 Elongation** % in 2 inch 18 **Test values are nominal approximations and depend on specimen size and orientation.Physical Properties
Thermal Conductivity BTU/ (sq ft-ft-hr-F) 22.3 Specific Heat BTU/lb/ºF @ 68F .09 Thermal Expansion Per °F from 68 F to 572 F .000009 Density lb/cu in @ 68 F .278 Electrical Conductivity % IACS @ 68 F 8 Modulus of Elasticity KSI 15,000 *Volume basis
Fabrication Practices
Stress relieving temperature | 600 F or 315 C |
Time at temperature | 1 hour per inch of section thickness |
Responds to heat treatment | Yes |
Solution heat treating temperature | 1600-1675 F or 870-910 C |
Time at temperature | 1 hour per inch of section thickness |
Quenching medium | Water |
Annealing temperature | 1150-1225 F or 620-660 C |
Time at temperature | 1 hour per inch of section thickness |
Machinability rating (Free Cutting Brass=100) | 60 |
Suitability for being joined by: | Soldering/Good |
Brazing/Good | |
Oxyacetylene Welding/Not Recommended | |
Gas Shielded Arc Welding/Good | |
Coated Metal Arc Welding/Fair |